CNC Turning for Stainless Steel 304
Turning 304 stainless requires constant chip engagement and sharp tooling. The material's work-hardening tendency makes it essential to never let the tool dwell or rub.
建議加工參數
| 參數 | 數值 |
|---|---|
| 可達公差 | ±0.02 mm (±0.0008") |
| 表面光潔度 | Ra 0.8-3.2 μm |
| 切削速度 | 100-200 m/min |
| 進給速率 | 0.10-0.25 mm/rev |
| 刀具建議 | Carbide inserts grade M20-M30 with TiAlN coating. Use chip-breaking geometry. Cermet for finishing. |
專家加工技巧
1
Never reduce feed below 0.05 mm/rev — the tool must cut, not rub
2
Use chip-breaking inserts always
3
High-pressure coolant directed at cutting zone
4
Replace inserts frequently — dull tools cause work-hardening
常見加工零件
Fittings and couplings
Valve stems
Medical device shafts
Food processing rollers
Fasteners
加工挑戰
- Severe work-hardening
- Stringy chips difficult to break
- Built-up edge formation
- High cutting temperatures